Investigation of Cathode Electrolyte Interphase Formation via Coupling Liquid Electrochemical TEM and GC/MS

Gallegos-Moncayo, Rezkallah, Jean et al.
A deeper understanding of the cathode electrolyte interphase (CEI) formation mechanism is essential to elucidate battery degradation. Here, we combine Liquid Electrochemical Transmission Electron Microscopy (ec-TEM) with Gas Chromatography/Mass Spectrometry (GC/MS) to monitor CEI evolution in a realistic electrochemical environment, focusing on electrolyte behavior under high voltages. The correlation between the electrochemical response, gas and liquid analysis after cycling, and the observation of deposited species on the working electrode (WE) reveals the processes governing CEI formation, stability, and composition. Cycling between 4 and 6 V vs Li leads to dispersed particles instead of a continuous film. These are partly composed of LiF and an amorphous phase that prevents dissolution at high potential. When cycled between 2.5 and 5.5 V, an anodic current peak indicates the formation of a 36 nm amorphous thin film without crystalline LiF, attributed to EC oxidation producing HF and subsequent LiF at a higher potential. LiF dissolution appears to follow a two-step pathway: electrolyte oxidation forms soluble intermediates, which are later reduced at lower potential to yield species capable of dissolving LiF. These results provide new insights into CEI formation and dissolution mechanisms, underscoring the need for further studies across different potential windows and with non carbonate electrolytes to validate these findings.
academic

Investigation of Cathode Electrolyte Interphase Formation via Coupling Liquid Electrochemical TEM and GC/MS

Basic Information

  • Paper ID: 2510.12467
  • Title: Investigation of Cathode Electrolyte Interphase Formation via Coupling Liquid Electrochemical TEM and GC/MS
  • Authors: Kevyn Gallegos-Moncayo, Josephine Rezkallah, Justine Jean, Arash Jamali, Grégory Gachot, Arnaud Demortière
  • Classification: physics.chem-ph
  • Institutions: CNRS LRCS Laboratory, RS2E Network, ALISTORE European Research Institute, et al.
  • Paper Link: https://arxiv.org/abs/2510.12467

Abstract

This study monitors the evolution of cathode electrolyte interphase (CEI) in authentic electrochemical environments by combining liquid electrochemical transmission electron microscopy (ec-TEM) and gas chromatography-mass spectrometry (GC/MS), with emphasis on electrolyte behavior at high voltages. The research reveals that cycling at 4-6V vs Li forms dispersed particles rather than continuous films, with these particles partially composed of LiF and amorphous phases that prevent dissolution at high potentials. During cycling at 2.5-5.5V, anodic current peaks indicate formation of a 36 nm thick amorphous film of crystalline-free LiF. LiF dissolution follows a two-step pathway: electrolyte oxidation generates soluble intermediates, subsequently reduced at low potentials to produce substances capable of dissolving LiF.

Research Background and Motivation

Problem Definition

The cathode electrolyte interphase (CEI) is a nanoscale layer formed by electrolyte oxidation at the positive electrode in lithium-ion batteries, critically affecting battery performance and lifespan. Compared to the extensively studied solid electrolyte interphase (SEI), the formation mechanism and composition of CEI remain insufficiently understood.

Research Significance

  1. Battery Degradation Mechanisms: CEI rupture or dissolution leads to reformation, affecting electrolyte and reducing battery lifespan
  2. High-Voltage Battery Requirements: High energy density batteries require operation at high potentials, making CEI understanding crucial
  3. Transition Metal Dissolution: CEI instability causes transition metal dissolution, affecting battery efficiency and safety

Limitations of Existing Methods

While conventional techniques such as XPS, SEM, and NMR can analyze CEI, they struggle to observe the dynamic CEI formation process in real electrochemical environments in situ. Comprehensive research methods combining microscopic structure observation with chemical composition analysis are lacking.

Research Motivation

Develop a correlative analysis method combining liquid electrochemical TEM and GC/MS to investigate CEI formation, stability, and composition change mechanisms under conditions approaching actual battery operation.

Core Contributions

  1. Methodological Innovation: First combination of liquid electrochemical TEM with GC/MS technology, enabling real-time observation and chemical analysis of CEI formation
  2. Mechanism Elucidation: Reveals the two-step mechanism of LiF formation and dissolution, explaining CEI morphology differences across voltage windows
  3. Structure Characterization: Precisely identifies crystalline phases (LiF, LiOH) and amorphous phases in CEI through 4D-STEM ACOM technology
  4. Electrolyte Oxidation Pathways: Proposes specific oxidation mechanisms of EC and DMC in LP30 electrolyte
  5. Voltage-Dependency Discovery: Demonstrates strong dependence of CEI morphology and composition on cycling voltage window

Detailed Methodology

Experimental Design

The study employs a micro-cell system containing top and bottom chips separated by Si₃N₄ windows with 150 nm spacing. A three-electrode configuration is used: working electrode (WE), reference electrode (RE), and counter electrode (CE).

Key Technology Integration

1. Liquid Electrochemical TEM (ec-TEM)

  • Equipment: Protochips liquid electrochemical sample holder
  • Function: Real-time observation of interfacial changes during electrochemical reactions
  • Advantages: Provides nanometer-scale spatial resolution for dynamic observation

2. Gas Chromatography-Mass Spectrometry (GC/MS)

  • Parameters: He carrier gas flow rate 1.5 mL/min, 70 eV EI ionization source
  • Function: Analyzes gaseous and liquid products after cycling
  • Detection: Identifies electrolyte oxidation/reduction products

3. 4D-STEM ACOM Analysis

  • Technique: Automated crystal orientation mapping
  • Parameters: 200 kV acceleration voltage, 0.7° precession angle
  • Function: Distinguishes crystalline and amorphous phases, determines phase composition

Experimental Conditions

Micro-cell Configuration

  • MB1: Glassy carbon (GC) working electrode, 3-6V vs Li cycling, scan rate 1 mV/s
  • MB2: Pt working electrode, 2.5-5.5V vs Li cycling, scan rate 3 mV/s
  • Electrolyte: LP30 (1M LiPF₆ in EC:DMC = 1:1)

Experimental Results

High Voltage Window Experiments (4-6V vs Li)

Morphological Features

  • Forms dispersed particles of 1-1.5 μm rather than continuous films
  • Particles primarily distributed at electrode edge regions
  • STEM-EDX shows F content ~73 at.%, O content ~15 at.%

Phase Composition Analysis

4D-STEM ACOM identifies:

  • Crystalline Phases: LiF and LiOH
  • Amorphous Phases: Organic residues, potentially related to CEI formation
  • Spatial Distribution: Coexistence of crystalline and amorphous phases within particles

Extended Voltage Window Experiments (2.5-5.5V vs Li)

Electrochemical Response

  • 4.77V Peak: Attributed to EC oxidation
  • 5.0V Peak: Attributed to DMC oxidation
  • 5.37V Peak: DMC soluble organic intermediate oxidation
  • Reduction Peak: -0.18 mA, related to reduction process

CEI Layer Characteristics

  • Forms 36 nm thick continuous amorphous film
  • Primarily composed of F and O elements
  • No detectable crystalline LiF phase
  • Minimal particle deposition on surface

GC/MS Chemical Analysis Results

Gaseous Products

  • CO₂ Peak: Prominent peak at 6.06 minutes, confirming major oxidation product
  • N₂, Ar, H₂O: From air contamination
  • No HF-related products detected: Possibly due to detection limit or rapid reaction

Liquid Analysis

  • No typical electrolyte reduction products detected
  • Supports oxidation-dominated reaction mechanism

Mechanism Analysis

DMC Oxidation Mechanism

  1. DMC loses electrons and CH₃⁺ ions
  2. CH₃⁺ reacts with PF₆⁻ generating PF₅ and CH₃F
  3. Further oxidation produces diradical intermediates
  4. Final decomposition yields CO₂ and ½O₂

EC Oxidation Mechanism

  1. EC molecule cleavage releases electrons and H⁺
  2. H⁺ combines with PF₆⁻ forming HF and PF₅
  3. Secondary oxidation of symmetric molecules
  4. Final products: CO₂, O₂, and HF

Two-Step Mechanism of LiF Formation/Dissolution

Step 1: Formation Phase

  • Electrolyte oxidation generates HF
  • HF combines with Li⁺ forming LiF
  • Insoluble products deposit forming CEI

Step 2: Dissolution Phase

  • Oxidation products migrate toward anode and undergo reduction
  • Reduction products migrate back to cathode
  • Alters LiF dissolution/precipitation equilibrium, promoting LiF dissolution

In-Depth Analysis and Discussion

Voltage Window Effects

High Voltage Window (4-6V)

  • LiF remains stable at high potentials
  • Forms mixed crystalline-amorphous CEI structure
  • Non-continuous dispersed particle morphology

Extended Voltage Window (2.5-5.5V)

  • Low potentials promote LiF dissolution
  • Forms pure amorphous continuous film
  • Uniform thickness approximately 36 nm

Evolution of Chemical Composition

Significant differences in CEI chemical composition exist under different voltage conditions:

  • F/O Ratio Variation: Reflects differences in LiF content
  • Crystalline Phase Disappearance: Low potential cycling causes LiF dissolution
  • Amorphous Phase Increase: Accumulation of organic oxidation products

Comparison with Literature

Zhang et al. observed nano-scale LiF layer formation in PC electrolyte; this study obtains similar results in EC/DMC systems, confirming the universality of carbonate oxidation-induced LiF formation.

Technical Innovation and Advantages

Methodological Innovation

  1. Multi-technique Correlation: TEM morphology observation + GC/MS composition analysis + electrochemical testing
  2. In Situ Dynamic Monitoring: Real-time observation in authentic electrochemical environments
  3. Multi-scale Characterization: Comprehensive analysis from atomic to micrometer scales

Technical Advantages

  1. High Spatial Resolution: Nanometer-scale CEI structure resolution
  2. Chemical Sensitivity: Precise elemental and phase composition analysis
  3. Dynamic Process Capture: Time-resolved CEI formation and evolution
  4. Authenticity: Conditions approaching actual battery operation

Limitations and Challenges

Experimental Limitations

  1. HF Detection: Direct HF detection not achieved due to detection limits or reaction speed issues
  2. Sample Size: Micro-cell systems may differ from actual batteries
  3. Voltage Accuracy: Pseudo-reference electrode may affect voltage measurement accuracy

Technical Challenges

  1. Sample Preparation: High requirements for TEM observation in liquid environments
  2. Data Correlation: Effective correlation and interpretation of multi-technique data
  3. Dynamic Processes: Real-time capture of rapid electrochemical reactions

Future Research Directions

Electrolyte System Expansion

  1. Non-carbonate Electrolytes: Verify universality of HF-driven LiF formation mechanism
  2. Additive Effects: Investigate electrolyte additive effects on CEI formation
  3. High-Concentration Electrolytes: Explore concentration effects

Technical Method Improvements

  1. Temporal Resolution Enhancement: Faster dynamic process capture
  2. Detection Sensitivity: Improved detection capability for critical intermediates like HF
  3. In Situ Spectroscopy: Integration with in situ Raman or infrared spectroscopy

Deeper Mechanism Investigation

  1. Temperature Effects: CEI formation mechanisms at different temperatures
  2. Current Density Influence: Charge/discharge rate effects on CEI
  3. Long-term Stability: CEI cycling stability and evolution patterns

Practical Application Value

Battery Design Guidance

  1. Voltage Window Optimization: Provides voltage range selection basis for high-voltage batteries
  2. Electrolyte Formulation: Guides selection of electrolyte components and additives
  3. Interface Engineering: Provides theoretical foundation for artificial CEI design

Industrial Application Prospects

  1. Battery Diagnostics: Development of rapid CEI state detection methods
  2. Lifespan Prediction: Battery lifespan models based on CEI evolution
  3. Quality Control: Interface quality monitoring in battery manufacturing

Conclusions

This study successfully establishes a correlative analysis method combining liquid electrochemical TEM and GC/MS, deeply revealing CEI formation mechanisms and evolution patterns. Major findings include:

  1. Voltage Dependency: CEI morphology and composition strongly depend on cycling voltage window
  2. Two-Step Mechanism: LiF formation and dissolution follow an electrolyte oxidation-intermediate migration-reduction dissolution pathway
  3. Complex Phase Composition: CEI comprises crystalline phases (LiF, LiOH) and amorphous organic phases
  4. Dynamic Equilibrium: CEI stability is determined by combined redox reactions and dissolution-precipitation equilibrium

These findings provide important insights into high-voltage lithium-ion battery interfacial chemistry, establishing a scientific foundation for developing more stable, high-performance battery systems. The methodological innovation and result depth provide valuable technical pathways and theoretical guidance for further development in this field.